United States Patent [191
`Itoh et al.
`
`IlllllllllllllIllllllllllllllllllllllllllllllllllllllllllllllllllllllllllll
`
`US005160998A
`[11] Patent Number:
`[45] Date of Patent:
`
`5,160,998
`Nov. 3, 1992
`
`[54] SEMICONDUCTOR DEVICE AND METHOD
`OF MANUFACTURING THE SAME
`[75] Inventors: Junichi Itoh, Inagi; Kazuyuki Kurita,
`Yokohama, both of Japan
`[73] Assignee: Fujitsu Limited, Kanagawa, Japan
`[21] App]. No.: 780,564
`[22] Filed:
`Oct. 21, 1991
`
`[63]
`
`Related US. Application Data
`Continuation of Ser. No. 233,108, Aug. 15, 1988, aban
`doned.
`Foreign Application Priority Data
`[30]
`Aug. 18, 1937 [JP]
`Japan .............................. .. 62-203483
`
`_ [51] Int. Cl.5 ........................................... .. H01L 29/34
`
`[52] US. Cl. . . . . . . . . . . . . . . . .
`
`. . . . . .. 257/760; 257/633
`
`[58] Field of Search . . . . . . .
`
`. . . .. 357/ 71, 54, 52, 40,
`357/65
`
`[56]
`
`References Cited
`U.S. PATENT DOCUMENTS
`
`4,135,954 1/1979 Chang et a1. ................... .. 357/54 X
`
`4,365,264 12/1982 Mukai et al. . . . . . . . . .
`4,446,194 5/1984 Candelaria et a1. .
`
`. . . .. 357/52 X
`.... .. 357/54
`
`4,455,568 6/1984 Shiota . . . . . . . . . . . . . .
`
`. . . .. 357/54
`
`4,654,689 3/1987 Fujii . . . . . . . . . . . . .
`
`. . . .. 357/40
`
`4,825,277 4/1989 Mattox et a]. .................. .. 357/54 X
`
`FOREIGN PATENT DOCUMENTS
`
`0152794 8/1985 European Pat. Off. ............ .. 357/71
`0252179Al 1/1988 European Pat. Off. .
`51-117887 10/1976 Japan .
`52-28870 3/1977 Japan .
`52-115785 9/1977 Japan .
`55-19850 2/1980 Japan .
`57-45931 3/1982 Japan .
`0190043 11/1983 Japan ................................... .. 357/71
`61-279132 12/1986 Japan .
`
`OTHER PUBLICATIONS
`Ghandhi, S. VLSI Fabrication Principles, John Wiley
`and Sons, 1983, pp. 582-585.
`Claassen, W. A. P. “Ion Bombardment-Induced Me
`chanical Stress in Plasma-Enhanced Deposited Silicon
`Nitride and Silicon Oxynitride Films.” Plasma Chemis
`
`try and Plasma Processing, vol. 7, No. 1 (Mar. 1987), pp.
`109-124.
`Machida, Katsuyuki and Hideo Oikawa. “New Planari
`zation Technology Using Bias-ECR Plasma Deposi
`tion.” Japanese Journal of Applied Physics. supplements
`17th Conf. on Solid State Devices and Materials Aug.
`25-27, 1985, pp. 329-332.
`Patent Abstracts of Japan, vol. 6, No. 119 (E-l16) [997],
`Jul. 3 1982; and JP-A-57 45 931 (Fujitsu K. K.) Mar. 16,
`1982.
`11, No. 138
`Patent Abstracts of Japan, vol.
`(E-503)[2585], May 2, 1987; and JP-A-61 279 132
`(Sony Corp.) Dec. 9, 1986.
`Extended Abstracts, vol. 87-1, No. 1, Spring 1987, pp.
`366-367, No. 254, Philiadelphia, Pa. U.S.; M. Doki et
`al.: “ECR Plasma CVD of Insulator Films-Low Tem
`perature Process for Ulsi-”.
`Patent Abstracts of Japan, vol. 11, No. 390 (15-567)
`[2837], Dec. 19, 1987; and JP-A-62 154 642 (Matsushita
`Electronics Corp.) Sep. 7, 1987.
`Primary Examiner-Andrew J. James
`Assistant Examiner-Sara W. Crane
`Attorney, Agent, or Firm-Nikaido, Marmelstein,
`Murray & Oram
`ABSTRACT
`[57]
`A semiconductor device including a semiconductor
`substrate; a metal wiring layer formed on the semicon
`ductor substrate; a ?rst insulation layer formed on the
`metal wiring layer, the ?rst insulation layer being
`formed by a tensile stress insulation layer having a con
`tracting characteristic relative to the substrate; and a
`second insulation layer formed on the ?rst insulation
`layer, the second insulation layer being formed by a
`compressive stress insulation layer having an expanding
`characteristic relative to the substrate. The tensile stress
`- insulation layer is produced by thermal chemical vapor
`deposition or plasma assisted chemical vapor deposition
`which is performed in a discharge frequency range
`higher than 2 megahertz; and the compressive stress
`insulation layer is produced by plasma assisted chemical
`vapor deposition which is performed in a discharge
`frequency range lower than 2 megahertz.
`
`5 Claims, 6 Drawing Sheets
`
`43.2
`
`33
`
`32
`
`422
`421
`
`412 411
`
`31
`
`MICRON ET AL. EXHIBIT 1050
`Page 1 of 12
`
`

`
`US. Patent
`
`Nov. 3, 1992
`
`Sheet 1 of 6
`
`5,160,998
`
`Fig.2
`Fig. l
`W
`Fig. 4
`
`M
`
`C
`% S
`
`S
`
`Fig. 3
`
`m S
`F/lTiMLLwL-T
`
`Fig. 6
`
`——> DISCHARGE FREQUENCY
`
`ICDkHz
`IIIIIIII
`I
`
`|
`
`1MHZ 2M
`
`lOM-lz
`I III‘
`
`I
`
`TENEILE
`
`x _..__. x
`
`-
`
`' / I ,
`X
`
`000
`
`1 1_-%
`
`520E520:
`wmwEm
`
`MICRON ET AL. EXHIBIT 1050
`Page 2 of 12
`
`

`
`US. Patent
`
`Nov. 3, 1992
`
`Sheet 2 of 6
`
`5,160,998
`
`'31
`
`Fig, 5(a)
`
`Fig. 5(b)
`
`I
`
`Fig. 5 (d)
`
`) m 5
`.9 H
`
`412 411
`
`31
`
`MICRON ET AL. EXHIBIT 1050
`Page 3 of 12
`
`

`
`US. Patent
`
`Nov. 3, 1992
`
`Sheet 3 of 6
`
`5,160,998
`
`' Fig. 7(a)
`
`I
`
`N
`
`31 %’2
`Fig. 7(b) \Fig.7(b’)
`%@ %f
`
`31
`
`411’
`
`31
`
`I
`‘ 4"
`
`Fig. 7(a)
`
`Fig. 7(c’)
`
`31
`
`412/’
`
`31
`
`+f412f
`
`Fig. 7 (d)
`
`Fig. 7(d')
`
`MICRON ET AL. EXHIBIT 1050
`Page 4 of 12
`
`

`
`US. Patent
`
`Nov. 3, 1992
`
`Sheet 4 of 6
`
`5,160,998
`
`Fig. 8(0)
`
`31
`r»?
`
`2
`
`Fig. 8(b)
`
`41
`“"2
`1
`
`Fig. 8 (c)
`
`Fig. 8 (f)
`iii/43 42
`
`33
`
`32
`31
`
`,
`
`2
`
`Fig, 8(9)
`
`14
`
`~ 1??“
`
`33 43
`42
`32
`31
`
`41
`2
`
`MICRON ET AL. EXHIBIT 1050
`Page 5 of 12
`
`

`
`US. Patent
`
`Nov. 3, 1992
`
`Sheet 5 of 6
`
`5,160,998
`
`Fig. 9
`
`w m
`
`1 5
`
`m0 O:.<m QMPQJDEDQUq
`
`
`
`
`.°\L ZO_P<mmZmO FUmEmD
`
`C
`
`I/A/
`Vim?
`A/A Q @/ /AM
`
`lt/XIV/Q @
`
`.D@ e A
`
`10
`
`TIME
`
`J
`50
`100
`(HOUR)
`
`500
`
`MICRON ET AL. EXHIBIT 1050
`Page 6 of 12
`
`

`
`US. Patent
`
`Nov. 3, 1992
`
`Sheet 6 of 6
`
`5,160,998
`
`x 0 k P P F P P H
`
`O Q Q 0 k P k F H
`
`X 0 P Q P L, P k a.
`
`0 o U P u P F P E
`
`0 u U P Q P Q P w
`
`9 .QE
`
`
`
`@635 “6 558 mlm Tm wrw Tm N-" I
`
`zo??mzwo $50 ozq
`
`$53155 205335
`
`33 EM:
`
`MICRON ET AL. EXHIBIT 1050
`Page 7 of 12
`
`

`
`SEMICONDUCTOR DEVICE AND METHOD OF
`MANUFACTURING THE SAME
`
`This application is a continuation of application Ser.
`No. 233,108 ?led Aug. 15, 1988, abandoned.
`
`III
`
`BACKGROUND OF THE INVENTION
`(1) Field of the Invention
`The present invention relates to a semiconductor
`device and a method of manufacturing the same. More
`particularly, it relates to an improvement of a semicon
`ductor device having metal wiring layers and insulation
`layers formed on the metal wiring layers, and an im
`provement of the method of manufacturing the same.
`(2) Description of the Related Art
`Generally, in the conventional semiconductor device
`of the above type, the insulation layers formed on the
`metal wiring layers (e.g., aluminum wiring layers) are
`produced by chemical vapor deposition using insulation
`material such as phosphor silicated glass (PSG).
`In this method, however, during the formation of the
`above insulation layers, problems have arisen such as a
`disconnection of the metal wiring layers due to stress
`migration due to the effect of stress generated in the
`insulation layers, and cracks in the insulation layers.
`The present invention is intended to solve the above
`mentioned problems, and the main object of the present
`invention is to effectively prevent not only the discon
`nection of the metal wiring layers due to stress migra
`tion but also a generation of cracks in the insulation
`layers.
`
`15
`
`20
`
`25
`
`SUMMARY OF THE INVENTION
`To attain the above-mentioned object, according to
`one aspect of the present invention, there is provided a
`semiconductor device comprising a semiconductor sub
`strate; a metal wiring layer formed on the semiconduc
`tor substrate; a ?rst insulation layer formed on the metal
`wiring layer, the ?rst insulation layer being formed by a
`tensile stress insulation layer having a contracting char
`acteristic relative to the substrate; and a second insula
`tion layer formed on the ?rst insulation layer, the sec
`ond insulation layer being formed by a compressive
`stress insulation layer having an expanding characteris
`tic relative to the substrate.
`Also, according to another aspect of the present in
`vention, there is provided a semiconductor device com
`prising a semiconductor substrate; a plurality of metal
`wiring layers formed on the semiconductor substrate,
`the plurality of metal wiring layers comprising one or
`more lower side metal wiring layers having a small
`wiring width and one or more upper side metal wiring
`layers having a large wiring width; one or more ?rst
`insulation layers formed on the respective lower side
`metal wiring layers , each of the ?rst insulation layers
`being formed by a tensile stress insulation layer having
`a contracting characteristic relative to the substrate;
`and one or more second insulation layers formed on the
`respective upper side metal wiring layers, each of the
`second insulation layers being formed by a compressive
`stress insulation layer having an expanding characteris
`tic relative to the substrate.
`In addition, according to the present invention, there
`are provided methods for manufacturing the above
`mentioned semiconductor devices.
`As above-mentioned, the tensile stress insulation
`layer has a contracting characteristic relative to the
`
`35
`
`45
`
`55
`
`65
`
`1
`
`5,160,998
`
`2
`substrate, and thus, when the tensile stress insulation
`layer T is formed on the semiconductor substrate S as
`shown in FIG. 1, the tensile stress insulation layer T
`causes the substrate S to bend in a direction such that
`the insulation layer T contracts relative to the substrate
`S (i.e., a direction such that the insulation layer T com- ,
`presses the metal wiring layer M formed on the sub
`strate S).
`On the other hand, the compressive stress insulation
`layer has an expanding characteristic relative to the
`substrate, and thus, when the compressive stress insula~
`tion layer C is formed on the semiconductor substrate S
`as shown in FIG. 2, the compressive stress insulation
`layer C causes the substrate S to bend in a direction such
`that the insulation layer C expands relative to the sub
`strate S (i.e., a direction such that the metal wiring layer
`M formed on the substrate S is expanded together with
`the insulation layer C when the metal wiring layer is
`heated by a current ?owing therethrough).
`Thus, according to one aspect of the present inven
`tion, by forming the tensile stress insulation layer T on
`the metal wiring layer M as the ?rst insulation layer, the
`insulation layer T applies stress to the metal wiring
`layer M, to compress the metal wiring layer as shown in
`FIG. 3, and as a result, a disconnection of the metal
`wiring layer due to stress migration is prevented. Also,
`by forming the compressive stress insulation layer C on
`the ?rst insulation layer T as the second insulation layer,
`as shown in FIG. 4, the compressive stress insulation
`layer tends to expand together with the expansion of the
`metal wiring layer when the metal wiring layer is
`heated, and thus the stress applied by the metal wiring
`layer to the insulation layer at that time is reduced, and
`as a result, a generation of cracks in the insulation layer
`is prevented.
`Also, according to another aspect of the present in
`vention, by forming the tensile stress insulation layers
`on the respective lower side metal wiring layers having
`a small wiring width (e.g., on the ?rst and the second
`metal wiring layers), a disconnection of the metal wir
`ing layers having a small wiring width due to stress
`migration is prevented. Also, by forming the compres
`sive stress insulation layers on the respective upper side
`metal wiring layers having a large wiring width (e.g.,
`on the third and the fourth metal wiring layers), a gen
`eration of cracks in the insulation layers due to the
`expansion of the metal wiring layers having a large
`wiring width is prevented. In this connection, with
`regard to the metal wiring layers having a large wiring
`width, a disconnection thereof due to stress migration
`need not be considered.
`As described in detail below, the tensile stress insula
`tion layer may be produced by thermal chemical vapor
`deposition (thermal CVD) or plasma assisted chemical
`vapor deposition (plasma CVD) performed in a dis
`charge frequency range higher than 2 megahertz. On
`the other hand, the compressive stress insulation layer
`may be produced by plasma assisted chemical vapor
`deposition (plasma CVD) performed in the discharge
`frequency range lower than 2 megahertz. Also, when
`the above tensile stress insulation layer or compressive
`stress insulation layer is formed by a particular plasma
`assisted chemical vapor deposition such that the above
`plasma is produced by electron cyclotron resonance
`(ECR plasma CVD), the surface of the corresponding
`insulation layer can be made flat, and thus ensure a high
`reliability of the metal wiring layers formed on the
`?attened surfaces of the insulation layers.
`
`MICRON ET AL. EXHIBIT 1050
`Page 8 of 12
`
`

`
`20
`
`25
`
`30
`
`35
`
`5,160,998
`3
`4
`tion of the metal wiring layer 31. Then, as shown in
`In this connection, US Pat. No. 4,446,194 discloses a
`method of forming a dielectric layer having a compres
`FIG. 5(c), a compressive stress insulation layer 412 is
`sive stress (corresponding to compressive stress insula
`formed as a second insulation layer on the tensile stress
`tion layer) on the metal layer and forming a dielectric
`insulation layer 411. In this connection, the compressive
`layer substantially free of compressive stress (corre
`stress insulation layer 412 expands together with the
`sponding to the tensile stress insulation layer) on the
`metal wiring layer 31 when the metal wiring layer is _
`compressive stress insulation layer, to prevent a forma
`heated by a current ?owing therethrough, due to the
`tion of voids in the metal layers.
`expanding characteristic thereof relative to the sub
`strate, and thus stress applied by the metal wiring layer
`But, as shown in the experimental data described in
`detail below, a semiconductor device according to the
`to the insulation layer at that time is reduced, and as a
`present invention (i.e., a semiconductor device compris
`result, a generation of ‘cracks in the insulation layer is
`prevented.
`ing a tensile stress insulation layer formed on the metal
`layer and a compressive stress insulation layer formed
`In this connection, the tensile stress insulation layer
`on the tensile stress insulation layer) effectively pre
`411 can be formed by thermal chemical vapor deposi
`vents both a disconnection of the metal layers due to
`tion (thermal CVD) or plasma assisted chemical vapor
`deposition (plasma CVD). When the thermal CVD
`stress migration and a generation of cracks in the insula
`tion layers, compared with the device disclosed in the
`method is used, the insulation material such as phosphor
`above U.S.P. Namely, according to present invention,
`silicated glass (PSG) or silicon dioxide (SlOz) is depos
`the above-mentioned particular advantages can be ob
`ited on the metal wiring layer under the condition of a
`tained, which cannot be expected from the above
`reduced atmospheric pressure or standard atmospheric
`U.S.P.
`pressure, and a processing temperature range higher
`than 200° C., preferably from 300° C. to 450° C. When
`the plasma CVD method is used, the insulation material
`(the reaction gas) such as the above PSG, SiOg, SiON,
`Si3N4 or BPSG (boron-phosphor silicated glass), is de
`posited on the metal wiring layer by supplying a high
`frequency power having the discharge frequency range
`higher than 2 megahertz (e.g., 13.56 megahertz) be
`tween ?at electrodes arranged, for example, in parallel,
`one of which electrodes is connected to the substrate,
`under the processing temperature range of from 200' C.
`to 450° C.
`The plasma CVD method is used for forming the
`compressive stress insulation layer 412, and the insula
`tion material (the reaction gas) such as the above PSG,
`SiOg, SiON, Si3N4, or BPSG is deposited on the ?rst
`insulation layer by supplying a high frequency power
`having a discharge frequency range lower than 2 mega
`hertz (e.g., 200 kilohertz) between the above electrodes,
`under a processing temperature range of from 200° C. to
`450° C.
`Note, the above plasma CVD is of a type other than
`a plasma CVD wherein the plasma is produced by elec
`tron cyclotron resonance (ECR plasma CVD) as de
`scribed below.
`FIG. 6 is a diagram showing how the value of the
`stress generated in the insulation layer produced by the
`plasma CVD is changed in accordance with a change in
`the discharge frequency of the high frequency power
`supplied from a high frequency generator connected
`between the above electrodes used in the plasma CVD
`system. In FIG. 6, the abscissa corresponds to the dis
`charge frequency, and the ordinate corresponds to the
`value of the stress (using 10'' dyne/cmz, where n=8 for
`PSG, and n=9 for Si3N4, as a unit) generated in the
`insulation layer produced by the plasma CVD. This
`plasma CVD was performed by using the insulation
`material (reaction gas) of the above PSG and Si3N4.
`The value of the tensile stress generated in the insula
`tion layer is represented as a positive value, and the
`value of the compressive stress generated in the insula
`tion layer is represented as a negative value.
`The value of the stress becomes zero at the point
`where the discharge frequency is 2 megahertz, and the
`value of above tensile stress increases in accordance
`with the increase of the discharge frequency in the
`frequency range higher than 2 megahertz. On the other
`hand, the value of the above compressive stress in
`
`BRIEF DESCRIPTION OF THE DRAWINGS
`FIG. 1 is a drawing explaining a characteristic of the
`tensile stress insulation layer;
`FIG. 2 is a drawing explaining a characteristic of the
`compressive stress insulation layer;
`FIG. 3 is a drawing showing the tensile stress insula
`tion layer formed on the metal wiring layer as a ?rst
`insulation layer;
`FIG. 4 is a drawing showing the compressive stress
`insulation layer formed on the ?rst insulation layer as
`the second insulation layer;
`FIGS. 5(a) to 5(e) are drawings showing a process for
`manufacturing a semiconductor device according to a
`?rst embodiment of the present invention;
`FIG. 6 is a diagram showing how the value of the
`stress generated in the insulation layer produced by the
`plasma CVD is changed in accordance with the change
`of discharge frequency used in the plasma CVD system;
`40
`FIGS. 7(a) to 7(d’) are drawings showing a process
`for manufacturing semiconductor devices according to
`second and third embodiments of the present invention;
`FIGS. 8(a) to 8(h’) are drawings showing a process
`for manufacturing a semiconductor device according to
`a fourth embodiment of the present invention;
`FIG. 9 is a diagram showing experimental data re
`garding the generation of stress migration in various
`cases; and
`FIG. 10 is a diagram showing experimental data re
`garding the generation of cracks in the insulation layers
`in various cases.
`
`45
`
`50
`
`55
`
`65
`
`DESCRIPTION OF THE PREFERRED
`EMBODIMENTS
`FIGS. 5(a) to 5(e) show a process for manufacturing
`a semiconductor device according to a ?rst embodi
`ment of the present invention. First, as shown in FIG.
`5(a), a ?rst metal wiring layer (e.g., aluminum wiring
`layer) 31 is formed on a semiconductor substrate 1 (e.g.,
`a silicon substrate) via a silicon insulation ?lm 2 (e.g., a
`silicon dioxide (SiOZ) ?lm). Next, as shown in FIG.
`5(b), a tensile stress insulation layer 411 is formed as a
`?rst insulation layer on the ?rst metal wiring layer 31.
`The tensile stress insulation layer 411 functions to com
`press the metal wiring layer 31, due to the contracting
`characteristic thereof relative to the substrate, and thus
`prevents stress migration which will cause a disconnec
`
`MICRON ET AL. EXHIBIT 1050
`Page 9 of 12
`
`

`
`15
`
`25
`
`35
`
`5,160,998
`5
`creases in accordance with a decrease of the discharge
`frequency in the frequency range lower than 2 mega
`hertz. Namely, the tensile stress insulation layer is
`formed when the plasma CVD is performed at the dis
`charge frequency range higher than 2 megahertz, and
`the compressive stress insulation layer is formed at the
`discharge frequency range lower than 2 megahertz.
`These conditions remain unchanged even when the
`above ECR plasma CVD is adopted, instead of another _
`type of plasma CVD, for forming the insulation layer.
`10
`Then, as shown in FIG. 5(a'), a second metal wiring
`layer 32 is formed on the second insulation layer 412.
`When the above~mentioned steps are repeated, a tensile
`stress insulation layer 421 and a compressive stress insu
`lation layer 422 are successively formed on the second
`metal wiring layer 32, and a third metal wiring layer 33
`is formed on the above insulation layer 422 correspond
`ing to the second insulation layer.
`Then, in the above embodiment, the compressive
`stress insulation layer 432 is formed as a cover on the
`third metal wiring layer 33, as shown in FIG. 5(e), and
`subsequently, an anneal processing for the semiconduc
`tor device is carried out for about half an hour under a
`temperature of, for example, 450° C.
`FIGS. 7(a) to 7(d') show a process for manufacturing
`semiconductor devices according to second and third
`embodiments of the present invention; the step shown in
`FIG. 7(a) corresponds to that of the above FIG. 5(a).
`Next, in the second embodiment of the present inven
`tion, as shown in FIG. 7(b), a tensile stress insulation
`layer 411' is formed on the ?rst metal layer 31 as the ?rst
`insulation layer. This insulation layer 411' may be
`formed by the same means as used to form the tensile
`stress insulation layer 411 in the ?rst embodiment.
`Then, as shown in FIG. 7(c), a compressive stress insu
`lation layer 412’ is formed as the second insulation layer
`on the ?rst insulation layer 411'. The insulation layer
`412' is formed so that the surface thereof is made ?at.
`In this connection, the insulation layer 412' having
`the ?attened surface is formed by the above-mentioned
`ECR plasma CVD method.
`In this case, this ECR plasma CVD is carried out
`under the condition that the microwave power for pro
`ducing the ECR Plasma is, for example, 800 watts, and
`the discharge frequency and the output of the high
`frequency bias power applied between one electrode
`connected to the substrate and the other electrode (e.g.,
`the earth electrode) are, for example, 400 kilohertz and
`50 to 100 watts, respectively. Namely, as shown in FIG.
`6, even when the above ECR plasma CVD is adopted,
`the compressive stress insulation layer may be produced
`in a discharge frequency range of the above bias power
`which is lower than 2 megahertz. Under this condition,
`the insulation layer 412' is produced by using an insula
`tion material such as SiO2, PSG, SiON, Si3N4 or BPSG.
`Accordingly, the surface of the insulation layer 412‘
`may be ?attened, and then, as shown in FIG. 7(d), a
`second metal wiring layer 32 formed on the ?attened
`surface of the insulation layer 412'. Further, the above
`steps for forming the ?rst and second insulation layers
`60
`and the metal wiring layer may be successively repeated
`a predetermined number of times.
`Also, in the third embodiment of the present inven
`tion, after the ?rst step shown in FIG. 7(a), as shown in
`FIG. 7(b'), a tensile stress insulation layer 411" is
`formed as the ?rst insulation layer on the ?rst metal
`wiring layer 31, in such a manner that the surface of the
`insulation layer 411” is made ?at.
`
`6
`As above-mentioned, the insulation layer 411" having
`a ?attened surface, is formed by the above ECR plasma
`CVD method. In this case, this ECR plasma CVD is
`carried out under the condition that the above micro
`wave power for producing the ECR plasma is, for ex
`ample, 800 watts, and the discharge frequency and the
`output of a high frequency bias power applied between
`the above electrodes, one of which electrodes is con
`nected to the substrate, are, for example, 13.56 mega
`hertz and 50 to 100 watts, respectively. Namely, as
`shown in FIG. 6, even when the above ECR plasma
`CVD is adopted, the tensile stress insulation layer may
`be produced in the discharge frequency range of the
`above bias power, which is higher than 2 megahertz.
`Under this condition, the insulation layer 411” is pro
`duced by using the insulation material such as PSG,
`SiOZ, SiON, Si3N4 or BPSG.
`Then, as shown in FIG. 7(c'), a compressive stress
`insulation layer 412" is formed as the second insulation
`layer on the ?attened surface of the insulation layer
`411". The insulation layer 412" may be formed by the
`same means used to form the compressive stress insula
`tion layer 412 in the ?rst embodiment. The surface of
`the insulation layer 412", which is formed on the ?at
`tened surface of the insulation layer 411" also may be
`?attened. Then, as shown in FIG. 7(d’), a second metal
`wiring layer 32 is formed on the ?attened surface of the
`insulation layer 412". Further, the above steps for form
`ing the ?rst and second insulation layers and the metal
`wiring layer can be successively repeated a predeter
`mined number of times.
`Thus, according to the second and third embodi
`ments of the present invention, since each of the metal
`wiring layers is formed on the ?attened surface of the
`corresponding insulation layer, a high reliability of the
`metal wiring layers is ensured.
`FIGS. 8(a) to 8(h’) show a process for manufacturing
`a semiconductor device according to a fourth embodi
`ment of the present invention. In this embodiment, a
`plurality of metal wiring layers are provided, the tensile
`stress insulation layer is formed on each of lower side
`metal wiring layers having a small wiring width, and
`the compressive stress insulation layer is formed on
`each of upper side metal wiring layers having a large
`wiring width.
`Namely, in this embodiment, the tensile stress insula
`tion interlayers 41 and 42 are formed on the ?rst and
`second metal wiring layers 31 and 32 having small wir
`ing widths l1 and 12, respectively, to prevent disconnec
`tion of the metal wiring layers having the small wiring
`widths due to stress migration. In this connection, the
`tensile stress insulation layers may be formed by the
`same means used to form the tensile stress insulation
`layers in the above ?rst embodiment.
`Also, the compressive stress insulation layers (inter
`layers and a cover) 43, 44, and 45 are formed on the
`third, fourth, and ?fth metal wiring layers 33, 34, and 35
`having large wiring widths l3, l4, and 15, respectively. In
`this connection, it is not necessary to consider discon
`nection of the metal wiring layers having the large
`wiring widths 13 to 15, due to stress migration. Accord
`ingly, as above-mentioned, the compressive stress insu
`lation layers are formed on the metal wiring layers
`having the large wiring widths, to prevent the genera
`tion of cracks in the insulation layers, due to expansion
`of the metal wiring layers having the large wiring
`widths. The compressive stress insulation layers also
`may be formed by the same means used to form the
`
`45
`
`50
`
`55
`
`65
`
`MICRON ET AL. EXHIBIT 1050
`Page 10 of 12
`
`

`
`15
`
`25
`
`5,160,998
`7
`8
`compressive stress insulation layers in the above ?rst
`layers is formed only by the tensile stress insulation
`embodiment.
`layer produced by thermal CVD, and marks “O”
`In this connection, in the above semiconductor de
`along a line “d” correspond to test data in the case
`vice having a plurality of metal wiring layers, one or
`wherein each of the insulation interlayers is formed only
`more metal wiring layers having the small wiring
`by the compressive stress insulation layer produced by
`widths (e.g., signal lines) are formed with a high wiring
`plasma CVD. Further, marks “El” along a line “b”
`density as the lower side metal wiring layers (in the
`correspond to test data in the case wherein each of the ’
`insulation interlayers comprises the compressive stress
`above case, as the ?rst and second metal wiring layers),
`and the remaining metal wiring layers having the large
`insulation layer as the ?rst insulation layer and the ten
`wiring widths (e.g., power supply lines) are formed
`sile stress insulation layer formed on the compressive
`with a low wiring density as the upper side metal wiring
`stress insulation layer as the second insulation layer, as
`layers (in the above case, as the third to ?fth metal
`shown in the above US. Pat. No. 4,446,194, and marks
`wiring layers).
`“A” along a line “a” correspond to test data in the case
`wherein each of the insulation interlayers comprises the
`In FIGS. 8(a) to 8(h’), the steps shown in FIG. 8(a)
`and FIG. 8(b) correspond to those of FIG. 5(a) and
`tensile stress insulation layer as the ?rst insulation layer
`FIG. 5(b), respectively.
`and the compressive stress insulation layer formed on
`Next, as shown in FIG. 8(0), the second metal wiring
`the tensile stress insulation layer as the second insulation
`layer 32 having the wiring width 12 is formed on the
`layer, as in the present invention.
`tensile stress insulation interlayer 41, and as shown in
`As shown in FIG. 9 it is apparent that the construc
`FIG. 8(d), the tensile stress insulation interlayer 42 is
`tion according to the present invention is remarkably
`effective for preventing stress migration, compared to
`again formed on the metal wiring layer 32. Next, as
`shown in FIG. 8(e), the third metal wiring layer 33
`other cases.
`having the wiring width 13, which is larger than the
`FIG. 10 shows experimental data regarding the gen
`‘above 11, and 12, is formed on the insulation interlayer
`eration of cracks in the insulation layers in various
`42, and as shown in FIG. 8(/), the compressive stress
`cases.
`insulation interlayer 43 is then formed on the metal
`In FIG. 10, test data I corresponds to the case
`wiring layer 33. Next, as shown in FIG. 8(g), the fourth
`wherein the insulation interlayers formed on the ?rst,
`metal wiring layer 34 having the wiring width 14, which
`second, and third metal wiring layers are all formed
`only by the tensile stress insulation layers T, and only
`is also larger than 11, and 12, is formed on the insulation
`interlayer 43. The above steps are repeated a predeter
`the cover formed on the fourth metal wiring layer is
`formed by the compressive stress insulation layer C.
`mined number of times, and ?nally, as shown in FIG.
`8(h), the compressive stress insulation layer 45 is formed
`Also, test data III corresponds to the case wherein the
`as the cover on the ?fth metal wiring layer 35 having,
`insulation interlayers formed on the ?rst and second
`for example, the wiring width 15 which is also larger
`metal wiring layers are formed only by the tensile stress
`than 11, and 12.
`insulation layers T, and the insulation interlayer formed
`FIG. 8(h') shows another typical construction of the
`on the third metal wiring layer comprises the compres
`semiconductor device according to the above fourth
`sive stress insulation layer C as a ?rst insulation layer
`embodiment of the present invention. This semiconduc
`3-1 of the corresponding insulation interlayer and the
`tor device comprises four metal wiring layers including
`tensile stress insulation layer T formed on the ?rst insu
`two lower side metal wiring layers (i.e., the ?rst and
`lation layer 3-1 as a second insulation layer 3-2 of the
`second metal wiring layers 31 and 32 having small wir
`corresponding insulation interlayer, as shown in the
`ing widths l1’ and 12', respectively) and two upper side
`above U.S.P., and the cover formed on the fourth metal
`metal wiring layers (i.e., the third and fourth metal
`wiring layer is formed by the compressive stress insula
`wiring layers 33 and 34 having large wiring widths l3’
`tion layer C. These test data I and III show that, accord
`and 14’, respectively). The tensile stress insulation inter
`ing to the above constructions, it is impossible to pre
`layers 41 and 42 are formed on the above lower side
`vent the generation of cracks in the insulation layers, as
`metal wiring layers 31 and 32, respectively, and the
`shown by marks “X”.
`compressive stress insulation layers (an interlayer and a
`On the other hand, test data II corresponds to the
`cover) 43 and 44 are formed on the above upper side
`case wherein the insulation interlayers formed on the
`metal wiring layers 33 and 34, respectively. The tensile
`?rst and second metal wiring layers (i.e., the metal wir
`ing layers having the small wiring width) are formed by
`stress insulation layers and the compressive stress insu
`the tensile stress insulation layers T, and the insulation
`lation layers may be formed by the same means used to
`form the tensile stress insulation layers and the compres
`interlayer formed on the third metal wiring layer and
`sive stress insulation layers in the above ?rst embodi
`the cover formed on the fourth metal wiring layer (i.e.,
`the insulation inter

This document is available on Docket Alarm but you must sign up to view it.


Or .

Accessing this document will incur an additional charge of $.

After purchase, you can access this document again without charge.

Accept $ Charge
throbber

Still Working On It

This document is taking longer than usual to download. This can happen if we need to contact the court directly to obtain the document and their servers are running slowly.

Give it another minute or two to complete, and then try the refresh button.

throbber

A few More Minutes ... Still Working

It can take up to 5 minutes for us to download a document if the court servers are running slowly.

Thank you for your continued patience.

This document could not be displayed.

We could not find this document within its docket. Please go back to the docket page and check the link. If that does not work, go back to the docket and refresh it to pull the newest information.

Your account does not support viewing this document.

You need a Paid Account to view this document. Click here to change your account type.

Your account does not support viewing this document.

Set your membership status to view this document.

With a Docket Alarm membership, you'll get a whole lot more, including:

  • Up-to-date information for this case.
  • Email alerts whenever there is an update.
  • Full text search for other cases.
  • Get email alerts whenever a new case matches your search.

Become a Member

One Moment Please

The filing “” is large (MB) and is being downloaded.

Please refresh this page in a few minutes to see if the filing has been downloaded. The filing will also be emailed to you when the download completes.

Your document is on its way!

If you do not receive the document in five minutes, contact support at support@docketalarm.com.

Sealed Document

We are unable to display this document, it may be under a court ordered seal.

If you have proper credentials to access the file, you may proceed directly to the court's system using your government issued username and password.


Access Government Site

We are redirecting you
to a mobile optimized page.





Document Unreadable or Corrupt

Refresh this Document
Go to the Docket

We are unable to display this document.

Refresh this Document
Go to the Docket